Masterbatch over powder is the preferred route on high-speed corrugation and extrusion lines: it gives dust-free dosing, clean dispersion, and lot-to-lot consistency of the antimony trioxide loading.
Carrier selection
- Use HDPE/MDPE-compatible carrier (LDPE/LLDPE or EVA-CPE) with MFI matched to the base resin within ±10–15% to avoid flow mismatch and short-shot/weld-line weak spots in thin walls.
- Declare carrier type and MFI on the CoA; a mismatched carrier raises plate-out at the corrugation mandrel and roughens the inner bore.
Dosing and halogen–antimony ratio
- Effective Sb2O3 dose: 3–5 wt% on the polymer fraction for rigid conduit, 4–6 wt% for flexible cable ducting grades.
- Target ~3:1 halogen:Sb. With chlorinated paraffin (CP-52/70) use Cl:Sb ≈ 3:1; with brominated FRs (DBDPE, brominated epoxy oligomers) retune to Br:Sb ≈ 3:1 computed on effective bromine, not compound weight.
- Optional zinc borate at 30–50% of the Sb2O3 loading for smoke suppression in building-service applications.
Processing controls
- Pre-dry 2–4 h at 70–80 °C when storage has exceeded 60% RH; residual moisture accelerates dielectric degradation in cable ducting.
- Keep melt temperature ≤ 190 °C (rigid PVC grades) / ≤ 200 °C (PE grades); monitor die, sizing sleeve and corrugation mandrel for plate-out every 2–4 h.
- Use screen-pack pressure rise and filter pressure as a dispersion proxy; fine grade D50 0.8–1.5 µm reduces white specks and bloom on both bore and outer wall.
Qualification checks
- Per-lot: dielectric strength, 7-day water-immersion insulation resistance (cable ducting), cold-bend at −20 °C, and reaction-to-fire class (EN 61386 / UL94) verified on the finished wall thickness, not on pellets.
- Confirm flexural/crush retention < 10% drop and heat-aging (135 °C / 168 h) retention within the acceptance window.
CoA requirements
- Purity ≥ 99.5%, moisture < 0.3%, Pb < 50 ppm, Fe < 100 ppm, D50 0.8–1.5 µm, whiteness ΔE < 1 per lot.
- Retain 200 g per lot for 12 months; CoA batch number ↔ test report ↔ retained sample ↔ lot archive traceable ≥ 5 years.
Qualify on a production run with end-product fire-class and cold-bend verification before committing a batch.