服务热线:
18971017202
您的位置:首页 >> 新闻中心

Sb2O3 Masterbatch for Fire-Retardant PET/rPET Staple Fibre & Filament

发布日期:2026-11-21 05:35:45   浏览量:0

1. Why masterbatch over powder for polyester fibre

  • Dust-free dosing on spinning lines: powder raises hygiene/explosion-dust concerns and gives uneven dispersion in 0.5–6 dtex filaments.
  • Lot consistency: masterbatch delivers stable Sb2O3 level + whiteness batch to batch, which matters for dye-lot and ΔE control of the yarn.
  • Carrier match: use a PET carrier of matching IV (intrinsic viscosity, e.g. 0.55–0.72) so the masterbatch co-crystallises with the base PET instead of forming weak spots.

2. Loading and halogen–antimony synergy

  • Dose effective Sb2O3 3–5 wt% on the polymer fraction (fibre FR grades rarely need more; higher loading degrades drawability).
  • Retune Br:Sb ≈ 3:1 on effective bromine when paired with brominated FR (e.g. brominated epoxy oligomer / BTBPE); do not calculate against compound weight.
  • Optional zinc borate 30–50% of the Sb2O3 weight for smoke suppression and a char-forming layer.
  • Target LOI ≈ 28–32% for polyester knit/woven at the finished fabric stage — verify on fabric, not on pellets.

3. Processing pitfalls

  • Pre-dry hard: PET hydrolyses above ~0.005% moisture — dry masterbatch + base blend to <0.005% (typically 130–150°C, 4–6 h) before spinning to avoid IV drop and filament breakage.
  • Melt window: keep processing ≤265°C (PET) to limit degradation and plate-out; monitor spinneret and draw-roller build-up (white residue = poor dispersion / wrong carrier).
  • Filter-pack pressure: a rising differential on the spinneret screen pack is the cheapest real-time dispersion proxy — log it per lot.
  • Fibre tenacity: after FR addition expect some tenacity loss; accept if drawability and tenacity stay within spec, else lower loading and re-tune synergy.

4. QC and CoA verification

  • CoA per lot: purity ≥99.5%, moisture <0.3%, D50 0.8–1.5 µm (fine grade, anti white-specks in thin filaments), Pb <50 ppm, Fe <100 ppm, whiteness ΔE <1.
  • Trial checks before committing a batch: dye-lot ΔE, filament tenacity/elongation, LOI + vertical burn on finished knit/woven, IV retention (<0.02 drop).
  • Heavy-metal migration (Sb, Pb) for apparel/hygiene-grade fibre — confirm within limits on the finished fabric.
  • Retained sample: 200 g per lot, 12 months; keep CoA ↔ batch number ↔ fabric test report traceability ≥5 years.

5. Supplier qualification

  • Masterbatch supplier must hold a fibre-grade CoA and be able to hold lot traceability to the spinning line; annual requalification and line-trial qualification are recommended.
在线咨询 联系方式 二维码

服务热线

18971017202

扫一扫,关注我们