Why Masterbatch for Impact-Critical Housing Grades
Power-tool bodies, battery-pack housings and handheld appliance shells are injection-moulded from ABS (often ABS/PC) or rigid PVC, and must pass both UL94 V-0 and pass a drop/impact test. Adding Sb2O3 as loose powder degrades toughness and leaves white specks at the thin walls. An ABS- or rigid-PVC-carrier Sb2O3 masterbatch keeps dispersion fine, metering exact and lot-to-lot consistency — the three things that hurt impact retention on tool housings.
Dose & Synergy Window (recalculate on effective halogen)
- Use effective Sb2O3 at 3–5 ph. phr (on 100 parts resin) for ABS; 3–5 phr for rigid PVC power housings.
- With a brominated FR (decabromodiphenyl ethane / brominated epoxy oligomer) target Br:Sb ≈ 3:1 on effective bromine; for chlorinated PVC bases use Cl:Sb ≈ 3:1 with chlorinated paraffin CP-52/70.
- Optional zinc borate at 30–50% of the Sb2O3 loading to cut smoke and afterglow without losing the V-0.
Carrier, Moisture & Processing Checks
- Match the masterbatch carrier to the resin polarity/MFI (ABS/SAN carrier for ABS; rigid-PVC K58-65 or EVA-CPE carrier for PVC).
- Pre-dry before moulding: ABS/PC 2–4 h at 80–90 °C, target moisture <0.02%; rigid-PVC pre-dry 2–4 h at 70–80 °C when storage >60% RH. Moisture is the #1 cause of splay/silver streaks that become crack-initiation points in drop tests.
- Keep melt below ~220 °C (ABS) / ≤190 °C (PVC); run a plate-out / mould-fouling check on long cycles and set a cleaning schedule.
- Dispersion QC: mould a 1.5–2.0 mm plaque, verify no visible specks and that notched-Izod/Charpy retains ≥85% of the unfilled control.
End-Product Qualification
- Run UL94 V-0 at the final wall thickness (usually 1.5–3.0 mm), not on thick bars.
- Add the tool-specific drop test from 1 m at −10 °C and a battery-crush/no-fire test if the part houses cells.
- Heat-age 70–105 °C 7 days; confirm no surface bloom (Sb2O3 migration) and gloss retention.
CoA Acceptance Checklist
Per lot require CoA stating: purity ≥99.5%, moisture <0.3%, particle size D50 0.8–1.5 µm (and D97), Pb <50 ppm, Fe <100 ppm, whiteness ΔE <1 vs reference. Keep a 200 g per-lot retained sample for 12 months; link CoA lot ↔ test report ↔ retained sample ↔ delivery batch for traceability ≥5 years. Line-trial qualify every new lot before batch commit; add annual requalification.