Sb2O3 for Polyolefin Cable Compounds: Synergy with Zinc Borate and Loading Levels
Antimony trioxide (Sb2O3) is the halogen synergist of choice for polyolefin (PE/PP) cable compounds. This guide summarizes practical loading and co-additive guidance for compounders and procurement teams.
Why Sb2O3 in cable compounds
- Halogen synergy: Sb2O3 converts halogen acids into volatile antimony halides that quench flame reactions in the gas phase.
- Cable-grade compounds typically combine a halogenated flame retardant with Sb2O3 rather than using either alone.
Typical loading windows
| Compound type |
FR system |
Typical Sb2O3 level |
| PE cable sheathing |
Decabromodiphenyl ethane |
5–8 phr Sb2O3 with 18–25 phr bromine FR |
| PP connectors/housings |
Brominated polystyrene |
4–7 phr Sb2O3 |
| HFFR (halogen-free) |
ATH/MDH only |
Not applicable — no halogen synergist |
Note: halogen-free systems do not benefit from Sb2O3; do not add it as filler.
Synergy with zinc borate
- Replacing 10–30% of the bromine FR with zinc borate can improve char formation and smoke suppression while keeping Sb2O3 at the lower end of the window.
- A common starting point: bromine FR / Sb2O3 / zinc borate ≈ 20 / 6 / 5 phr, then optimize by LOI and UL 94 V-0 testing.
Procurement checkpoints
- Purity ≥ 99.5%, white degree consistent with agreed standard.
- Particle size / D50 in line with the compound's dispersion and color requirements.
- Ask for per-lot certificate of analysis and halogen-synergy trial data where available.
Summary: For polyolefin cable compounds, start with 5–8 phr Sb2O3 against a brominated FR, consider partial zinc borate substitution for smoke control, and verify each lot's purity and fineness before release.