Halogen-antimony synergy works in polyamides, but PA66's high processing temperature (280-300 degrees C) is close to Sb2O3-driven degradation limits.
Recommended dosage windows
- PA66 with brominated styrene or decabromodiphenyl ether: 12-16% brominated FR paired with 5-7% Sb2O3 typically reaches UL94 V-0 at 1.6 mm.
- Raising Sb2O3 above 8% rarely improves ratings but sharply increases melt viscosity and glass-fiber wet-out problems.
Processing care
- Avoid residence time longer than 8-10 minutes; secondary degradation releases bromine species that accelerate equipment corrosion.
- Use barrel temps at the lower end of the PA66 window and purge thoroughly before shutdown.
- Color stability: nylon discoloration is more sensitive to iron content in Sb2O3; specify Fe < 200 ppm for electrical-grade PA66.
Glass-fiber grades need slightly more Sb2O3 (about +1%) because glass dilutes the flame-retardant package.