服务热线:
18971017202
您的位置:首页 >> 新闻中心

Sb2O3 in Polycarbonate (PC): Transparency Limits and Alternatives

发布日期:2026-11-21 05:34:22   浏览量:0

Antimony trioxide is rarely usable in unfilled polycarbonate: with aromatic bromine sources such as brominated polycarbonate oligomers or tetrabromobisphenol-A carbonate oligomers, the bromine-antimony couple attacks the carbonate backbone and accelerates hydrolysis, which destroys both transparency and mechanical properties.

Where Sb2O3 still appears in PC

  • Opaque or dark PC blends (PC/ABS alloys) tolerate the halogen-antimony system because the discoloration is masked and the ABS phase carries the fracture risk.
  • For PC/ABS housings rated UL94 V-0 at 1.6 mm, typical formulations run 10-14% bromine source with 3-5% Sb2O3, confirmed by lab burns on the actual resin lot.
  • When transparency is required, specifiers switch to potassium diphenylsulfone sulfonate (KSS) or siloxane-based PC grades, which need no antimony at all.

Mechanical and degradation notes

  • Even in blends, hydrolytic attack scales with processing moisture; pre-dry PC/ABS at 100-110°C for 3-4 hours before compounding.
  • Excess antimony lowers heat-deflection temperature measurably; keep Sb2O3 against the minimum bromine ratio that passes burn testing, not the maximum.

Procurement checklist for PC/ABS molders

  1. Confirm the grade is low-iron, low-lead; iron catalyzes the same carbonate-hydrolysis yellowing.
  2. Require per-lot particle size distribution (D50 typically 0.8-1.5 micrometers for blend dispersion).
  3. Ask whether the supplier's grades have been burn-tested in PC/ABS references, not only PP or ABS.
  4. Pilot on the molder's own drying and screw profile before committing to annual volumes.