Sb2O3 Masterbatch for WPC Boardwalk Decking: Deck boards see foot traffic and rain pooling, so moisture uptake matters. Pre-dry pellets at 80°C for 2-4h if storage RH exceeded 60%. Use PE/PP carrier matched to the composite matrix (MFI 5-12 for extruded deck boards); dose 4-6% Sb2O3 with halogen source (DBDPE) at Br:Sb ~3:1 molar on polymer fraction. Fine-grade D50 0.8-1.5µm prevents surface specks on visible walking faces. Twin-screw compounding at 170-190°C; watch screen pack pressure rise (plate-out indicator). CoA checkpoints: purity ≥99.5%, moisture <0.3%, Pb <50ppm. Qualify each lot with a short extrusion trial checking surface gloss uniformity and flex strength; retain 200g sample per lot for 12 months against weathering complaints. Antimony trioxide masterbatch, WPC boardwalk, PE carrier, halogen-antimony synergy, plate-out control.