Application: Flame-retardant clear PET/PC films, sheets and thermoformed blister trays (electronics packaging, appliance fascia, lighting diffusers) where transparency and surface quality must be retained alongside a reaction-to-fire rating.
Carrier & Resin Matching
- Use a PET/PC-compatible carrier: co-polyester or clear-PET carrier for PET film (matched intrinsic viscosity IV ≈ 0.72–0.80), or a low-MFI clear PC/SAN carrier for PC sheet. Carrier polarity and refractive index should be close to the base resin to minimise haze.
- Avoid generic LDPE/EVA carriers in clear film: refractive-index mismatch raises haze and creates visible specks.
- Verify carrier MFI within 10–15% of the base resin to avoid surging or draw-line thickness variation on the cast/blown film line.
Halogen–Antimony Synergy
- Dose 2.5–4 wt% effective Sb2O3 (on polymer fraction) with a Br:Sb ≈ 3:1 molar ratio — use brominated aromatic FRs (DBDPE, brominated epoxy oligomers, brominated polystyrene) whose refractive index is compatible with clear film.
- Retune the ratio when the halogen source changes; chlorine-based systems shift the window and raise haze.
- For PC, watch carbonate-backbone hydrolysis — pre-dry the masterbatch and base resin to <0.02% moisture before melt processing.
Processing & Quality Control
- Pre-dry 2–4 h at 110–130 °C (PET) or 90–110 °C (PC) when storage RH > 60% — residual moisture causes haze, silver streaks and IV drop (embrittlement).
- Keep melt temperature in the resin's stable window; watch die/roll plate-out and bloom on clear film — fine grades (D50 0.8–1.5 µm) reduce white specks and surface bloom.
- Run haze/transmittance trial plaque (target haze < 2–3% at target thickness) and filter pressure / screen-blockage monitoring before batch commitment.
Supplier Qualification & CoA Checks
| Parameter |
Acceptance |
| Purity (Sb2O3) |
≥ 99.5% |
| Moisture |
< 0.3% |
| Particle size D50 |
0.8–1.5 µm (fine grade) |
| Pb / Fe |
< 50 ppm / < 100 ppm |
| Whiteness |
consistent per lot (≥ 96) |
| Refractive index match |
low-haze carrier confirmed |
- Require per-lot CoA and 200 g retained sample per lot for 12 months for traceability and dispute arbitration.
Verification Before Commit
- UL94 V-0 / VTM-0 at final wall thickness plus EN 13501-1 (or FMVSS 302 for automotive) on the finished film/sheet.
- Optical + mechanical checks (haze, transmittance, tensile, elongation) on thermoformed parts.
- Per-lot retained sample enables re-test if a downstream complaint arises.