Sb2O3 Masterbatch for EPDM/EPR Peroxide-Cured Cable Insulation

发布日期:2026-11-21 05:35:31   浏览量:0

Application Context

EPDM/EPR cable insulation is peroxide (DCP) or silane crosslinked. Adding an antimony trioxide (Sb2O3) masterbatch raises the fire-retardant performance but must not disturb the cure kinetics or the electrical/thermal balance of the compound.

Carrier & Dosing

  • Carrier: EPDM/EPR pellet carrier with matched Mooney viscosity (ML1+4 100°C within ±15 units) so the masterbatch disperses without over-shearing the rubber backbone.
  • Effective Sb2O3 dose: 3–5 phr on polymer fraction; retune the halogen:antimony ratio to ~3:1 Br:Sb (or Cl:Sb) when used with chlorinated paraffin / brominated co-additives.
  • Masterbatch loading: 40–60% Sb2O3 in the EPDM carrier, compounded on a two-roll mill or internal mixer; verify dispersion by filter-press / visual streak check on a thin sheet.

Cure-Interference Check (Critical)

  • Peroxide-cured systems: run a moving-die rheometer (MDR) t90 delta-time check. Reject line if t90 shifts >10–15% vs the non-flame-retardant control.
  • Antimony can scavenge radicals at high doses; keep the effective Sb2O3 within the recommended window to avoid under-cure or surface tackiness.

Flame & Electrical QC

  • LOI (limiting oxygen index) and vertical-burn per IEC 60332-1 on finished insulation (not compound alone).
  • Dielectric strength ≥ target kV/mm per-lot; insulation-resistance check after 7-day water immersion (moisture pickup raises conductivity).
  • Cold-bend −20°C and heat-aging 135°C/168h retention <10% drop for mechanicals.

CoA Verification (per lot)

  • Purity ≥ 99.5% Sb2O3
  • Moisture < 0.3% (moisture raises blister/void risk in steam-cure)
  • Particle size D50 0.8–1.5 µm (coarse grades hurt dielectric & cause lumps)
  • Pb < 50 ppm, Fe < 100 ppm
  • Whiteness consistency ΔE < 1 (visible on thin wall)

Process Notes

  • Pre-dry masterbatch 2–4 h at 70–80°C when storage RH > 60% before compounding.
  • Watch for plate-out / die build-up; adjust with fine-particle grade if bloom appears.
  • Retain 200 g per lot for 12 months for traceability and dispute arbitration.