Glass-reinforced PBT (15–30% GF) electronics connectors demand tight control when adding antimony trioxide:
Why masterbatch over powder - Pre-dispersed PBT/PET-carrier pellets avoid agglomerates at GF junctions and filter-pack blocking on small-shot molds. - Frees handling dust on high-cavitation tooling.
Dosing & synergy - Effective Sb2O3 3–5 wt% calculated on the resin fraction (not total including GF). - Brominated co-FR (brominated epoxy/PS oligomers) retuned to ~3:1 Br:Sb on the effective bromine; GF addition dilutes both — compensate 10–15%.
Processing - Pre-dry PBT and masterbatch 120–140 °C to moisture <0.02 % — PBT hydrolyzes rapidly above 250 °C melt, dropping IV and impact. - Melt ≤255 °C; watch die plate-out and screen pressure rise. - UL94 V-0 retest must be on final GF-filled wall thickness, never on neat resin plaques.
CoA qualification per lot - Purity ≥99.5 %, moisture <0.3 %, D50 0.8–1.5 µm, Pb <50 ppm, Fe <100 ppm, whiteness ΔE<1.
Retain 200 g per lot for 12 months; run an annual line requalification.