Why masterbatch over powder in rigid PUR foam? Polyurethane foam is produced by high-pressure/high-throughput impingement mixing of polyol with isocyanate. Powdered Sb2O3 metered into the polyol stream tends to settle, bridge and dose erratically, causing cell-wall pinholes, scorched faces and lot-to-lot FR scatter. A carrier-based masterbatch (reactant-compatible polyol dispersion, 40–60% Sb2O3) stays suspended, meters steadily through the recirculation loop and eliminates dust at the foaming machine.
Carrier selection
- Use a polyol-carrier slurry whose OH number and viscosity match the formulation polyol within ±10–15%; otherwise the masterbatch alters the stoichiometric -NCO index and the foam never gels on time.
- Compatibility red line: the carrier must be isocyanate-stable and not bleed-freezing agents that shift the cream/gel time by >10–15%.
- Fine grade D50 0.8–1.5µm prevents the coarse particles that sit at cell windows and punch holes in thin 30–50mm facer skins.
Dose & formulation window
- Effective Sb2O3 3–5 wt% on the polymer fraction (not on total foam density) with Br:Sb ≈ 3:1 by effective bromine from the FR polyol / TCPP-adjacent brominated additive — never by compound weight alone.
- Pair with zinc borate 30–50% of Sb2O3 weight for surface char reinforcement and reduced smoke. Higher boron load improves char but increases viscosity — verify pumpability before committing.
- Overdose check: above ~6 phr effective the foam gets brittle and the facer adhesion drops (peel loss). Sift-dose ladder on trial buns, not on production.
Moisture & processing
- Pre-dry: all polyol-side moisture must be <0.3% (ideally <0.2%) — residual water competes with isocyanate, blows CO2 instead of crosslinking, lowers core density and turns the flame test into a funnel test.
- Melt/process: isocyanate index 105–120; cream time shift test per masterbatch lot — a shift >10–15% flags carrier contamination; check gel time window on trial buns.
- Blowing-agent watch: pentane/HFC blowing interacts with over-dispersed additives (cell-wall puncture, low closed-cell %); re-run closed-cell content (ASTM D6226) per lot, keep ±5% of the reference bun.
End-product verification
- FR on the finished board/faced panel, not on the raw bun: UL94 (HB/V-0 per facing structure), EN 13501-1 (B/C class per density), and NFPA 285 / FM 4880 where a rainscreen assembly is required.
- Mechanical integrity: compressive strength (ASTM D1621) retained ≥85% at target density; dimensional stability 70°C/95%RH 7d growth <5% and -20°C no cold-fracture.
- Smoke/toxicity: EN 13501-1 s2/s3 smoke class and (rail/mining) NFF 16-101 / EN 45545 HL if specified — zinc borate helps here.
CoA per lot
Purity ≥99.5%, moisture <0.3%, D50 0.8–1.5µm, Pb<50ppm, Fe<100ppm, whiteness ΔE<1, carrier OH/viscosity declared. 200g retained sample 12 months; batch ↔ CoA ↔ bun-trial ↔ board-lot traceability ≥5 years; annual requalification.