服务热线
18971017202
For compounders of wire and cable insulation and sheathing, antimony trioxide (Sb2O3) remains the default synergist for brominated flame retardant systems. Getting the grade and loading right balances flame performance against insulation resistance and elongation at break.
Sb2O3 works by volatilizing with the halogen source to form antimony halides and oxyhalides that quench flame radicals in the gas phase. The classic benchmark ratio is 3:1 halogen to antimony by weight — for example, 15 phr bromine with 5 phr Sb2O3 in a PVC sheath or an EVA-based HFFR-adjacent system. For cable compounds you typically stay within a 2.5:1 to 3.5:1 window; going below 2:1 wastes halogen, going above 4:1 adds cost and ash without measurable LOI gains.
| Compound type | Typical Sb2O3 phr |
|---|---|
| Flexible PVC insulation | 4–7 |
| Flexible PVC sheathing | 6–10 |
| EVA/XLPE low-smoke sheath | 3–6 |
| TPE/TPO jackets | 3–5 |
Water absorption is the most common failure mode: uncoated Sb2O3 modestly raises moisture uptake, which can pull down insulation resistance after hot-water immersion testing. Use treated grades and validate against the relevant IEC/UL immersion requirement. Also check elongation at break after dry and wet thermal aging — over-compounding with synergy filler is the usual cause of brittle aged samples.
Before signing off a Sb2O3 lot for cable production: confirm CoA values for Sb2O3 ≥ 99.5% (or the grade's specified purity), lead and iron limits within spec, particle size distribution (D50 report), and white grade color consistency for pigmented compounds. Run a pilot compound at the target loading to confirm LOI, smoke density (EN 50268-2 or equivalent) and aged mechanical properties before final purchase orders.