服务热线
18971017202
Rigid PVC siding and cladding extrusions usually run 3-5 phr of flame-retardant antimony trioxide on the polymer fraction, paired with chlorinated paraffin or another halogen source at roughly 3:1 Cl:Sb.
Extrusion and dispersion. Carrier-match the masterbatch to rigid PVC (no plasticizer, declared K-value) and keep D50 in the 0.8-1.5 µm range so the profile surface stays free of white specks and plate-out. Two-roll mill check before trial, then die-pressure and vacuum-sizing watch on the line.
Coatings and weathering. Profiles that get painted or co-extruded need QUV/xenon results against the paint supplier's adhesion spec; plate-out at the die shows up first as coating defects after weathering.
Supplier qualification. CoA per lot: purity ≥99.5%, moisture <0.3%, Pb <50 ppm, whiteness consistent. Run gloss, impact and Vicat on a trial profile, and keep a 200 g retained sample per lot for 12 months.