PVC wall panels and wainscoting are interior decorative extrusions where flame retardancy must not compromise surface finish, embossing definition, or long-term whiteness. Adding Sb2O3 masterbatch to these profiles calls for attention to both the formulation and the shop-floor process.
Formulation notes - Rigid PVC wall panel bodies typically carry 3–5 phr Sb2O3, tuned with the halogen source (often chlorinated paraffin CP-52/70) to keep a roughly 3:1 halogen-to-antimony molar ratio on the compound. - For laminated or co-extruded panels with a soft PVC top layer, the cap layer dose should be trimmed 1–2 phr below the body to avoid surface bloom and embossing fill-in. - Pair with a Ca-Zn stabilizer system; verify with your stabilizer supplier that the masterbatch carrier does not disturb lubricant balance.
Processing checkpoints - Melt temperature kept at or below 190°C; higher zones accelerate brominated co-additive degradation and plate-out on calender rolls and embossing plates. - Check embossing roll for deposits every 2–4 hours of production; early plate-out shows up first as loss of wood-grain definition. - Pre-dry the masterbatch when storage humidity exceeds 60% RH to prevent silver streaks on glossy panel surfaces.
Supplier qualification - CoA per lot: purity ≥99.5%, moisture <0.3%, D50 0.8–1.5 µm, Pb <50 ppm, whiteness consistency against agreed standard. - Run a trial extrusion checking gloss uniformity, embossing sharpness, and impact strength before committing to batch orders. - Request a 200 g retained sample per lot, held for 12 months, tied to the shipment batch number for traceability.